Krems an der Donau, Austria
Purpose of this study was to investigate the mechanical efficiency of 3D-printed permanent and provisional implant cemented fixed bridges produced via CAD/CAM technology using an interim and a permanent ceramic filled hybrid material.
Two groups with twenty specimens each were designed and 3D-printed via digital light processing technology (DLP). A fracture strength test was performed. Statistical analysis was performed (p>0.05) for impression distance and force.
For the fracture resistance and impression distance no significant difference (p = 0.643) were detected. The specimens of interim resin showed a mean value of 365.90 ± 86.67 N. Whereas specimens of permanent ceramic filled hybrid material showed a mean value of 363.45 ± 87.57 N.
In this in vitro study 3D-printed ceramic filled hybrid material and interim resin based on methacrylic acid esters showed an acceptable resistance to bite forces with no differences in fracture mechanism.
© 2001-2025 Fundación Dialnet · Todos los derechos reservados